Natural colourants can be compounded into polylactic acid (PLA) and polybutylene succinate (PBS) on conventional twin-screw equipment without disturbing melt flow or mechanical performance, but whether they survive depends on the processing temperature of the polymer they are carried in, and their long-term colour stability remains unresolved. Those are the boundaries drawn by a study titled "Sustainability in the Development of Natural Pigment-Based Colour Masterbatches and Their Application in Biopolymers", which tested four commercial natural pigments in both biopolyesters as concern grows over the sustainability profile of conventional colorants.
The pigments were blue spirulina, yellow curcumin, red beetroot and green chlorophyllin. Each was combined with PLA and with PBS to produce colour masterbatches by twin-screw extrusion, then diluted into the matching polymer matrix at 2, 4 and 6 wt% and injection moulded into test specimens. The masterbatch formulations also contained titanium dioxide, calcium carbonate and stearic acid, added to support UV protection, pigment dispersion and processing.
Thermal degradation sets the processing window
The central difficulty is that natural colorants are organic structures that begin to break down at temperatures below those at which the carrier polymers soften and flow. Thermogravimetric analysis placed the degradation onset at roughly 229 °C for spirulina, 244 °C for curcumin, 258 °C for chlorophyllin and 267 °C for beetroot, while PLA and PBS degrade at considerably higher temperatures. That leaves a narrow band in which the polymer can be melted while the pigment is exposed to as little heat as possible.
The researchers built temperature profiles around that constraint: processing temperatures reached 145 °C for PBS and 190 °C for PLA, with the twin-screw extruder running at 65 rpm and a feed rate of 2 kg/h. The window proved wide enough for most pigment–polymer combinations, but not for all of them.
Spirulina reveals that the matrix matters as much as the pigment
The clearest failure was spirulina in PLA. Under the 190 °C PLA profile the pigment lost its characteristic blue, and no blue PLA masterbatch could be produced. The same pigment survived compounding in PBS, whose lower processing temperature preserved enough of it for successful masterbatch production. The result is a direct demonstration that pigment compatibility is a property of the pigment–matrix pair rather than of the pigment alone: a colorant that is workable in one biopolymer may be unusable in another solely because of the temperatures that matrix requires.
Rheology and mechanical behaviour stay close to baseline
From a processing standpoint the pigments proved undemanding. Melt flow rate fell only slightly after incorporation, indicating a modest rise in melt viscosity; neat PLA measured about 50 g/10 min and the corresponding natural-pigment masterbatches stayed near that figure, with PBS showing a comparable small reduction.
That matters for compounders. A natural colour system that forced major changes to screw design, pressure settings or moulding conditions would offer little practical value, whereas these formulations ran through conventional twin-screw compounding and injection moulding without major processing problems.
Mechanical properties were similarly stable across the 2 to 6 wt% addition range. PLA started from a Young's modulus of about 1710 MPa and a tensile strength of 65.6 MPa; PBS started from about 392 MPa and 34.5 MPa. The coloured formulations remained close to those baselines, and impact strength stayed within a similar range, although individual pigments introduced some variation.
Light, rather than heat, is the larger obstacle
Successful extrusion did not translate into durable colour. After 50 hours of xenon-lamp exposure, most formulations showed a colour difference above ΔE* = 2, the level at which a change becomes visually perceptible. The main exception was the PLA formulation containing 2 wt% of the green chlorophyllin masterbatch, which showed the highest photostability in the set.
The study therefore identifies UV stability as the largest barrier to broader use. Packaging, consumer products, agricultural parts and outdoor applications would need additional stabilisation, protective coatings or pigment modification before natural colours could compete with conventional systems over long service periods. Thermal stability during processing, though manageable inside the selected windows, likewise remains a development target.
An environmental case built on modelled assumptions
The work also compared the pigments' environmental footprint. Under its assumptions, one kilogram of curcumin pigment corresponded to about 0.04 kg CO2-eq, against 18.65 kg CO2-eq for the inorganic green reference pigment, and the natural-pigment masterbatches drew less electricity during extrusion and pelletising. These are modelled figures tied to the study's own assumptions rather than a complete life-cycle verdict, and are best read as an indication of direction rather than a settled comparison.
What the results do and do not establish
The contribution of the work is to show that several natural colorants can be compounded into PLA and PBS on standard equipment with only limited shifts in melt viscosity and mechanical performance, and that the binding constraints sit at the two ends of the service life: thermal exposure during processing and colour retention during use. Natural-pigment masterbatches therefore look technically feasible for a range of biopolymer applications, but they are not yet drop-in replacements. Lightfastness and thermal stability still require development, and pigment selection has to be matched to the processing temperature of the specific matrix rather than chosen on colour alone.